Swapping sintered NdFeB (Br around 1.15 to 1.30 T) for sintered ferrite (Br around 0.40 T) on a surface-magnet rotor doesn't go well. Air-gap flux drops to roughly 0.30 T, and to make up the torque the motor has to grow a lot.
The usual fix is a spoke rotor with tangentially magnetized ferrite. Each steel pole shoe sits between two magnet faces, so the flux concentrates in the gap. I've been writing worked examples for a book on analytical PM motor design. One of them sizes a 12-slot/10-pole and a 12-slot/14-pole motor to the same spec. I assumed the results would be close. They weren't.
The spec:
- 2.0 Nm continuous, 6.0 Nm peak for 2 s
- 3000 rpm base, 4500 rpm max
- 48 V DC bus, fan-cooled, envelope OD of 100 mm or less
- Rotor OD 63.0 mm, stack 40.1 mm (sized at a shear stress of 8 kPa), air gap 0.50 mm
- Ferrite: Br = 0.40 T at 20 °C (0.354 T at 80 °C), μr = 1.10, HcJ = 252 kA/m at -20 °C, magnet thickness 6.0 mm
Both slot/pole combos have the same fundamental winding factor (0.933), so on paper you could pick either one. That changed once I ran the magnetic circuit and the voltage check:
Parameter |12s10p |12s14p |Why
Pole pitch / pole arc ratio |19.8 mm / 0.697 |14.1 mm / 0.576 |More poles means less flux per pole
Magnet depth for Bg = 0.40 T |13.1 mm |7.7 mm |41% less radial depth needed
Hub radius left inside the magnets |17.4 mm |22.8 mm |Room for a stiffer shaft
Tooth width (loaded, Bt = 1.41 T) |6.2 mm |3.5 mm |Each 14p tooth only ever sees one pole's flux
Turns per coil (to pass the 48 V check) |8 |9 |The ωLq·iq drop dominates
Cold demag ratio, Hm/HcJ at -20 °C, full -id |0.96 (marginal) |0.83 (OK) |Armature MMF per pole scales as 1/p
Cogging periods per rev, LCM(Q, 2p) |60 |84 |Smaller, higher-frequency detents
Efficiency at 2 Nm, 3000 rpm |90.8% |90.7% |About the same, even at 350 Hz vs 250 Hz Three things that tripped me up, and probably trip up other people too:
1. The standard tooth-width formula. wt = Bg·τs / (Bt,max·kstk) assumes several teeth share one pole, i.e., τs ≤ αi·τp. In the 14-pole design, that isn't true. The slot pitch is 16.76 mm, and the pole arc is only 8.14 mm, so a tooth can never collect more than one pole shoe's flux. Use w_eff = min(τs, αi·τp) instead. If you plug in τs, your teeth come out 2.06 times too wide, and you lose slot area you actually need.
2. Checking demag at the hot corner. That habit comes from NdFeB. Ferrite runs the other way: coercivity rises with temperature (about +0.25 %/K), and remanence falls (about -0.19 %/K). The worst case is cold. At -20 °C, Br is highest, and HcJ is lowest. Check that corner first.
3. Ignoring armature reaction in the teeth. Spoke pole shoes sit right at the gap. On a surface-magnet rotor, the magnet adds tm/μr to the effective gap, but here there's nothing in the way. So q-axis armature reaction ends up about as strong as the magnet field. Loaded tooth flux goes up by k_arm = √(1 + (B_arm/B_g1)²), which is about 1.41 when the two are equal. The 0.4 T gap field is also why the loaded tooth sits at 1.41 T.
Has anyone here built a 12s14p ferrite spoke motor and checked cold demag on the bench? I'd like to know how close the analytical numbers came to what you measured.
Full disclosure: this comes from a book I just finished, Analytical Design of Brushless Permanent-Magnet Motors. It covers inner-rotor SPM, outer-rotor SPM, and ferrite spoke machines, plus nonlinear reluctance networks and when to hand a design off to FEA. A free sample PDF is up on Leanpub if you want to check the equations: https://leanpub.com/analyticaldesignofbrushlesspermanent-magnetmotors